ASTM and SAE reference for carbon, mild, aluminized and stainless tubes
Technical procurement and manufacturing reference | 17 November 2026 | Units: mm, MPa, mass % unless stated otherwise
Purpose and interpretation
This guide connects raw-material/coil designations with specifications for finished tubes. A grade alone does not define a compliant tube: the purchase order must also identify product form, applicable edition, dimensions, tolerance class, delivery condition, testing, inspection and documentation. Tables are curated commercial grade families, not a reproduction of copyrighted standards or an assertion that every grade ever standardized is included.
Important conformity principle
A comparison such as ASTM 304 ≈ EN 1.4301 ≈ a GOST chromium–nickel grade is a screening aid only. Chemical limits, deoxidation, stabilization, mechanical requirements, permitted processes, heat treatment and tests can differ. Never print an untested alternative standard on an MTC, and never treat a flat-sheet standard as finished-tube certification.
Standards register and applicability
Standard
Applies to
Commercial interpretation
ASTM A1008/A1008M
Cold-rolled uncoated carbon and HSLA sheet
Raw strip: CS, DS, DDS, EDDS, SS and HSLA families
ASTM A1011/A1011M
Hot-rolled carbon/structural/HSLA sheet and strip
Raw strip: CS, DS, SS grades, HSLA; thickness dependent
ASTM A568/A568M
General requirements for steel sheet, carbon and HSLA
Sheet ordering, tolerances, common requirements
ASTM A463/A463M
Continuously hot-dip aluminum-coated steel sheet
Type 1 Al–Si and Type 2 Al; coating & base steel grades
ASTM A924/A924M
General requirements for metallic-coated sheet
Referenced requirements and dimensions for coated sheet
ASTM A240/A240M
Cr and Cr–Ni stainless flat products
Sheet/strip for 300/400 stainless substrates
ASTM A480/A480M
General requirements for stainless flat products
Dimensions, finish and ordering requirements
ASTM A513/A513M
ERW carbon and alloy mechanical tubing
Common mechanical/exhaust tube route; type/grade must be stated
ASTM A500/A500M
Structural carbon tube, round or shaped
Load-bearing welded or seamless structural tubing
ASTM A53/A53M
Black or hot-dip zinc-coated welded/seamless steel pipe
Conveyance/ordinary piping; Grade A/B
ASTM A106/A106M
Seamless carbon-steel pipe for high-temperature service
High strength and weight reduction; verify formability
ASTM A36
Structural carbon plate/shapes
Not a universal tube-coil or tube standard
ASTM A500 Grade B/C/D
Structural hollow sections
Final tube grade with specified mechanical properties
ASTM A53 Grade A/B
Pipe grade
Pipe pressure/hydro requirements, not equivalent to A513
Why DC01 is not an American grade
DC01 belongs to EN 10130. US cold-rolled commercial/drawing steel is ordered through ASTM A1008/A1008M CS/DS/DDS/EDDS (or to a qualified SAE chemistry where specified). A US CS grade is not certified to DC01 unless tested and documented to both standards; tensile, yield, elongation and surface/aging requirements must all be reviewed.
Aluminized steel and coating options
ASTM A463 designation
Type / role
Technical or ordering consideration
CS Type A, B, C
Commercial forming
Type 1 or Type 2 coating per grade and order
FS
Forming Steel
Improved formability; verify edition availability
DDS
Deep Drawing Steel
More severe draw operations
EDDS
Extra Deep Drawing Steel
Very demanding drawing; supplier availability
SS Grades 33, 37, 40, 50 etc.
Structural
Exact grade/class permitted by edition
HSLAS Type A and B
High-strength low-alloy
Grade strength and class per specification
FSS 409 and 439
Ferritic stainless substrate
Coated stainless option: distinct from coated carbon
T1-13 / T1-20 / T1-25 / T1-40 / T1-60
Type 1 coating mass in oz/ft², both sides
Confirm available designation/edition; T1-40 ≈ 122 g/m²
T1M 40 / 60 / 75 / 100 / 120 / 150 etc.
Type 1 metric coating mass
Mass in g/m² combined both sides; confirm listed designation
T2-100
Type 2 predominantly aluminum coating
Different purpose, adhesion and appearance; no silent switch
Type 1 is an aluminum–silicon alloy coating intended for oxidation and heat resistance. Type 2 is substantially pure aluminum and differs in coating properties. ASTM Type 1 T1-40 uses approximately 0.40 oz/ft² total both faces, equivalent to approximately 122 g/m²; EN AS120 is near it by coating mass, not automatic full equivalence. Numeric coating values are mass, not minimum local thickness.
300 series stainless grade register
AISI / trade
UNS
EN screening cross-reference
Main tube relevance
Indicative chemistry, not acceptance limits
301
S30100
1.4310 X10CrNi18-8
austenitic; high work hardening; formed parts
Cr 16–18; Ni 6–8; C ≤0.15
302
S30200
1.4319 (comparison only)
austenitic; higher C than 304
Cr 17–19; Ni 8–10; C ≤0.15
303
S30300
1.4305 X8CrNiS18-9
free-machining; sulfur; poor welding choice
Cr 17–19; Ni 8–10; S ≥0.15
304
S30400
1.4301 X5CrNi18-10
general welded tube and fabrication
Cr 18–20; Ni 8–10.5; C ≤0.08
304L
S30403
1.4307 / 1.4306
lower carbon; welded assemblies
Cr 18–20; Ni 8–12; C ≤0.03
304H
S30409
1.4948 (check product)
elevated temperature; controlled carbon
C 0.04–0.10; Cr 18–20; Ni 8–11
305
S30500
1.4303 X4CrNi18-12
deep forming; higher nickel
Cr 17–19; Ni 11–13
309S
S30908
1.4833 X12CrNi23-13
heat oxidation service
Cr 22–24; Ni 12–15; C ≤0.08
310S
S31008
1.4845 X8CrNi25-21
heat-resistant high chromium nickel
Cr 24–26; Ni 19–22; C ≤0.08
316
S31600
1.4401 X5CrNiMo17-12-2
molybdenum for chloride resistance
Cr 16–18; Ni 10–14; Mo 2–3
316L
S31603
1.4404 / 1.4432 / 1.4435
welded chemical and hygienic tubes
C ≤0.03; Cr 16–18; Mo 2–3
316Ti
S31635
1.4571 X6CrNiMoTi17-12-2
Ti stabilized; hot service
Cr 16.5–18.5; Ni 10.5–13.5; Mo 2–2.5
317L
S31703
1.4438 (comparison only)
higher Mo; aggressive service
Cr 18–20; Ni 11–15; Mo 3–4
321
S32100
1.4541 X6CrNiTi18-10
Ti stabilized exhaust and heat
Cr 17–19; Ni 9–12; Ti controlled
347
S34700
1.4550 X6CrNiNb18-10
Nb stabilized weld/thermal applications
Cr 17–19; Ni 9–13; Nb controlled
904L
N08904
1.4539 X1NiCrMoCu25-20-5
high alloy austenitic; acid service
Cr 19–23; Ni 23–28; Mo 4–5; Cu 1–2
The chemistry column gives orientation ranges rounded from widely used specifications; acceptance requires the precise grade and edition’s chemical tables, product analysis tolerances and any agreed dual certification. EN variants under one US commercial name may have nonidentical nickel or molybdenum bounds.
400 series stainless grade register
AISI / trade
UNS
EN screening cross-reference
Main tube relevance
Indicative chemistry, not acceptance limits
405
S40500
1.4002 X6CrAl13
Al-alloyed ferritic stainless; distinct from coated steel
The 400 series spans ferritic and martensitic alloys. 409, 430, 439, 441 and 444 are ferritic; 410 and many 420 variants are martensitic. They cannot be substituted by series number alone. Stabilization is essential to welding and heat-resistance performance.
Special study 409AL and aluminized stainless
Two different uses of a similar name
In exhaust purchasing, “409AL”, “409 Aluminized” or “aluminized 409” commonly describes a 409 ferritic stainless substrate with hot-dip Al–Si coating (often Type 1), supplied as coated strip under ASTM A463/A463M or an agreed equivalent manufacturing specification. In other metallurgical contexts “409Al” may designate an aluminum-stabilized ferritic alloy rather than a surface-coated product. The suffix AL is not a safe stand-alone specification or universally standardized UNS grade.
Check
Required PO or MTC statement
Substrate
UNS S40900 / other explicitly specified 409 family grade; separate heat analysis
Coating
Al–Si Type 1 vs pure-Al Type 2; applicable sheet standard or mill technical specification
Coating mass
Exact T1 / T1M or EN AS designation, total-both-sides vs per-side convention
Finished tube
Tube standard, process (ERW, TIG/laser), OD, wall and length tolerances
Weld
Treatment of weld seam and local coating loss; corrosion qualification if required
Verification
Coating mass/thickness; adhesion; substrate PMI; tube dimensional and leak tests
A 409 substrate with aluminized coating is neither plain aluminized carbon steel nor bare 409 stainless. The coating may be damaged or absent at the weld seam and cut ends; agree on treatment and service testing. The producer should specify coating condition after tube forming, not only before it.
SAE carbon steel composition engineering cards
Grade
Nominal C %
Nominal Mn %
Material behavior
Quotation caveat
1006
≤0.08
0.25–0.40
Very soft / forming
Exact limits per SAE J403
1008
≤0.10
0.30–0.50
Cold formability and ERW
Exact grade/heat chemistry
1010
0.08–0.13
0.30–0.60
Weldable tube feedstock
Confirm residual elements
1015
0.13–0.18
0.30–0.60
General purpose low-carbon
Temper and process matter
1018
0.15–0.20
0.60–0.90
Machining and tube stock
Forming more limited
1020
0.18–0.23
0.30–0.60
Low-carbon engineering
Mechanical properties by tube norm
1026
0.22–0.28
0.60–0.90
Stronger mechanical tube stock
Weld requirements greater
1045
0.43–0.50
0.60–0.90
Heat-treatable medium carbon
Avoid unspecific ERW claim
Composition bands are practical SAE J403 screening values, not an authoritative quotation of a specified revision. SAE 1008 and 1010 may have multiple industry chemistry practices. The finished tube performance changes strongly with ERW, DOM, cold work and heat treatment.
ASTM A463 aluminized coating mass detailed comparison
US designation
Coating family
Total both-face coating mass minimum
Approximate metric equivalent
T1-13
Type 1 Al–Si
0.13 oz/ft²
40 g/m²
T1-25
Type 1 Al–Si
0.25 oz/ft²
76 g/m²
T1-40
Type 1 Al–Si
0.40 oz/ft²
122 g/m²
T1-60
Type 1 Al–Si
0.60 oz/ft²
183 g/m²
T1M 40
Type 1 Al–Si
40 g/m²
~0.13 oz/ft²
T1M 120
Type 1 Al–Si
120 g/m²
~0.39 oz/ft²
1 oz/ft² ≈ 305.15 g/m². Coating designation mass convention, sampling and minimum single-spot requirements must be checked in ASTM A463/A463M edition. Manufacturer data: Cleveland-Cliffs Aluminized Type 1 Product Data (2025). Type 1 typically contains about 9–11% silicon in the aluminum coating alloy.
US product mechanical requirements are not interchangeable
Cold-worked tempers can increase strength greatly; annealed values must not be applied to half-hard/full-hard strip.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4310 X10CrNi18-8) and corrosion exposure.
Tube production considerations
Strong work hardening; control rolling and tube-forming strain.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
302 stainless steel S30200
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 17–19; Ni 8–10; C ≤0.15
Mechanical properties
Mechanical properties depend on annealed or cold-worked temper.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4319 (comparison only)) and corrosion exposure.
Tube production considerations
Higher carbon means evaluate weld sensitization.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
303 stainless steel S30300
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 17–19; Ni 8–10; S ≥0.15
Mechanical properties
Mechanical strength depends on product form and temper.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4305 X8CrNiS18-9) and corrosion exposure.
Tube production considerations
Sulfur addition improves machinability but reduces fusion-weld suitability.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
304 stainless steel S30400
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 18–20; Ni 8–10.5; C ≤0.08
Mechanical properties
Typical solution-annealed plate/sheet minimum: Rp0.2 ~205 MPa; Rm ~515 MPa; elongation ~40% under common ASTM flat-product conditions. These figures are NOT universal finished-tube limits.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4301 X5CrNi18-10) and corrosion exposure.
Tube production considerations
TIG/laser or qualified ERW; assess seam corrosion, ID bead, and sensitization.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
304L stainless steel S30403
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 18–20; Ni 8–12; C ≤0.03
Mechanical properties
Typical annealed flat-product minima often Rp0.2 ~170 MPa, Rm ~485 MPa, A ~40%; verify actual product-standard edition.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4307 / 1.4306) and corrosion exposure.
Tube production considerations
Low carbon preferred for welded parts; 304/304L dual certificate requires both chemistries and all mechanical requirements.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
304H stainless steel S30409
Specification field
Technical requirement / engineering guidance
Chemical composition
C 0.04–0.10; Cr 18–20; Ni 8–11
Mechanical properties
High-temperature grades require carbon control and elevated-temperature design values.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4948 (check product)) and corrosion exposure.
Tube production considerations
Not interchangeable with 304L; confirm thermal service and heat treatment.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
305 stainless steel S30500
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 17–19; Ni 11–13
Mechanical properties
Cold-forming optimized; yield/tensile depend on condition.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4303 X4CrNi18-12) and corrosion exposure.
Tube production considerations
Excellent deep formability; check availability of tube coil.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
309S stainless steel S30908
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 22–24; Ni 12–15; C ≤0.08
Mechanical properties
Heat-resistant austenitic; strength is condition and temperature dependent.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4833 X12CrNi23-13) and corrosion exposure.
Tube production considerations
Oxidation/thermal cycling design matters more than generic room-temperature strength.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4845 X8CrNi25-21) and corrosion exposure.
Tube production considerations
High alloy weld consumable and thermal expansion considerations.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
316 stainless steel S31600
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 16–18; Ni 10–14; Mo 2–3
Mechanical properties
Common annealed flat-product minima: Rp0.2 ~205 MPa, Rm ~515 MPa, A ~40%; do not apply to every tube product.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4401 X5CrNiMo17-12-2) and corrosion exposure.
Tube production considerations
Mo enhances pitting resistance; not immune to chloride stress corrosion.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
316L stainless steel S31603
Specification field
Technical requirement / engineering guidance
Chemical composition
C ≤0.03; Cr 16–18; Mo 2–3
Mechanical properties
Common annealed flat-product minima: Rp0.2 ~170 MPa, Rm ~485 MPa, A ~40%; verify product-specific requirements.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4404 / 1.4432 / 1.4435) and corrosion exposure.
Tube production considerations
Lower carbon for welded corrosion service; surface passivation may be specified.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
316Ti stainless steel S31635
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 16.5–18.5; Ni 10.5–13.5; Mo 2–2.5
Mechanical properties
Condition, temperature and specimen direction determine applicable mechanical minima.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4571 X6CrNiMoTi17-12-2) and corrosion exposure.
Tube production considerations
Ti stabilized; specify solution treatment and avoid assuming same chemistry as 316L.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
317L stainless steel S31703
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 18–20; Ni 11–15; Mo 3–4
Mechanical properties
Higher Mo chemistry; mechanical values require exact product specification.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4438 (comparison only)) and corrosion exposure.
Tube production considerations
Corrosion qualification should match chloride/acidity environment.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
321 stainless steel S32100
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 17–19; Ni 9–12; Ti controlled
Mechanical properties
Common annealed flat-product tensile minimum around 515 MPa; full yield/elongation require edition.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4541 X6CrNiTi18-10) and corrosion exposure.
Tube production considerations
Titanium stabilization and weld heat exposure make treatment critical.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
347 stainless steel S34700
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 17–19; Ni 9–13; Nb controlled
Mechanical properties
Stabilized Cr–Ni steel; property limits depend on standard and condition.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4550 X6CrNiNb18-10) and corrosion exposure.
Tube production considerations
Nb stabilization; specify temperature cycling, weld process and test plan.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
904L stainless steel N08904
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 19–23; Ni 23–28; Mo 4–5; Cu 1–2
Mechanical properties
High alloy austenitic; minimum properties are product- and condition-specific.
Supply and metallurgical condition
Austenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4539 X1NiCrMoCu25-20-5) and corrosion exposure.
Tube production considerations
High Ni/Mo/Cu content; demanding weld qualification and PMI.
Inspection, test and certificate
Use ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precision
Indicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.
405 stainless steel S40500
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 11.5–14.5; Al 0.10–0.30
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
Al-alloyed ferritic stainless; distinct from coated steel; match exact UNS and EN designation (1.4002 X6CrAl13), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
Ti stabilized; exhaust components; match exact UNS and EN designation (1.4512 X2CrTi12), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
409L stainless steel S40910 / EN variant
Specification field
Technical requirement / engineering guidance
Chemical composition
Exact chemistry depends designation
Mechanical properties
Lower interstitial chemistry; properties depend on exact UNS and strip anneal.
Supply and metallurgical condition
low-C exhaust; check grade-specific producer chemistry; match exact UNS and EN designation (1.4512 comparison), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
410 stainless steel S41000
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 11.5–13.5; C ≤0.15
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
martensitic; may be heat treated; match exact UNS and EN designation (1.4006 X12Cr13), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
410S stainless steel S41008
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 11.5–13.5; C ≤0.08
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
low-C ferritic counterpart; match exact UNS and EN designation (1.4000 X6Cr13), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
420 stainless steel S42000
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 12–14; C varies materially
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
martensitic; wear/hardness applications; match exact UNS and EN designation (1.4021 / 1.4028 variants), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
17% chromium; household/ducting; match exact UNS and EN designation (1.4016 X6Cr17), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
430Ti stainless steel varies
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr ~16–18; Ti controlled
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
stabilized ferritic; specify exact designation; match exact UNS and EN designation (1.4510/1.4520 comparison only), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
434 stainless steel S43400
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 16–18; Mo ~0.75–1.25
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
Mo-bearing ferritic corrosion upgrade; match exact UNS and EN designation (1.4113 X6CrMo17-1), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
436 stainless steel S43600
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 16–18; Mo ~0.75–1.25
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
Mo-bearing and stabilized exhaust option; match exact UNS and EN designation (1.4526 comparison), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
Ti stabilized; exhaust and exchangers; match exact UNS and EN designation (1.4510 X3CrTi17), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
dual stabilized Ti+Nb; elevated-temp exhaust; match exact UNS and EN designation (1.4509 X2CrTiNb18), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
444 stainless steel S44400
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 17–20; Mo 1.75–2.5
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
Mo-bearing ferritic; high corrosion resistance; match exact UNS and EN designation (1.4521 X2CrMoTi18-2), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
446 stainless steel S44600
Specification field
Technical requirement / engineering guidance
Chemical composition
Cr 23–27
Mechanical properties
Mechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical condition
high-Cr oxidation resistance; match exact UNS and EN designation (1.4749 comparison), anneal/temper, surface finish and stabilization.
Tube production considerations
Ferritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificate
Order to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precision
Chemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.
Tube purchase-order specification matrix
Field
What an engineering inquiry or PO must state
Product
Welded round tube; intended mechanical, exhaust, heat-exchanger or pressure duty
Base grade
Exact material designation and source sheet/strip standard + edition
Applicable finished-product norm and edition; do not infer from strip grade
Dimensions
OD x nominal wall x cut length; tolerances, eccentricity, straightness, ovality
Production
HF-ERW / laser / TIG; weld-bead treatment; anneal/pickling/passivation if relevant
Verification
Chemistry, tensile or hardness, flattening/flaring/bend, leak/eddy/UT where applicable
Certification
EN 10204 3.1 or other agreed inspection certificate; heat/coil/tube traceability
Packing
Blue-wrapped bundles, without pallet/sleeve/slings if requested; moisture protection
Tube manufacturing and acceptance checks
Coil receipt
Record heat number, coil number, coating face/mass, thickness, tensile condition and supplier MTC. A tube made from a compliant coil is not automatically a compliant tube.
Slitting and forming
Confirm strip edge condition, strip width, springback, seam orientation, and coating crack tolerance. High-strength sheet may have limited formability.
Weld process
Identify HF-ERW, TIG or laser; assess weld speed and heat input, seam bead and heat-affected region. High-Cr ferritic tubes need controlled welding and may require post-weld treatment.
Dimensional checks
Measure OD, nominal and minimum wall, out-of-roundness, length, straightness, end squareness and bend/ovality where specified. Use the actual tube standard tolerances.
Nondestructive/leak testing
Apply the specific test prescribed or agreed for the product: eddy-current, ultrasonic, pneumatic or hydrostatic. An inspection technology is not a substitute for the required acceptance level.
Marking and documentation
Record manufacturer, standard, grade, size, batch/heat and inspection results. Any claim to ASTM, EN or GOST should be supported by all relevant mandatory tests.
Example ASTM purchase descriptions
ERW mechanical carbon tube, ASTM A513/A513M [edition], Type [ ], steel grade [SAE 1010 or agreed], OD 101.6 x WT 1.5 x L 3000 mm, condition [ ], dimensional tolerances [ ], eddy-current and MTC as agreed.
Aluminized exhaust tube, ASTM A463/A463M [edition] Type 1 CS Type B T1M 120 coil, formed into ERW tube to customer tube drawing / agreed tube product standard, OD 127 x WT 1.5 x L 5800 mm, welded-seam coating condition and bend test specified.
Welded stainless mechanical tube, ASTM A554 [edition], UNS S30400, OD 114.3 x WT 1.5 x L 1198 mm, finish and bead conditions agreed; ASTM A240 sheet certificate supplied additionally when required.
Aluminized 409 exhaust tube: ASTM A463 Type 1 FSS 409 substrate (confirm edition and exact UNS) with coating designation [ ], finished-tube requirements [ ]; separate substrate and coating test reports.