Shaped for Precision. Built for Industry.

Materials Standards

Russian GOST Steel and Tube Standards

GOST and GOST R reference with grade comparison and coating limitations

Technical procurement and manufacturing reference | 17 November 2026 | Units: mm, MPa, mass % unless stated otherwise

Purpose and interpretation

This guide connects raw-material/coil designations with specifications for finished tubes. A grade alone does not define a compliant tube: the purchase order must also identify product form, applicable edition, dimensions, tolerance class, delivery condition, testing, inspection and documentation. Tables are curated commercial grade families, not a reproduction of copyrighted standards or an assertion that every grade ever standardized is included.

Important conformity principle

A comparison such as ASTM 304 ≈ EN 1.4301 ≈ a GOST chromium–nickel grade is a screening aid only. Chemical limits, deoxidation, stabilization, mechanical requirements, permitted processes, heat treatment and tests can differ. Never print an untested alternative standard on an MTC, and never treat a flat-sheet standard as finished-tube certification.

Standards register and applicability

StandardScopeUse in a technical offer
GOST 380-2005Ordinary-quality carbon steel gradesSt0–St6 family; verify deoxidation suffix
GOST 1050-2013Quality nonalloy structural steel08, 10, 15, 20, 35, 45 etc.
GOST 9045-93Low-carbon cold-rolled sheet for cold stampingDrawing categories, not DC-grade direct equivalents
GOST 16523-97Thin sheet carbon steel general-quality/qualityFlat sheet technical requirements
GOST 19903-2015Hot-rolled sheet dimensionsNot a material grade
GOST 19904-90Cold-rolled sheet dimensionsNot a material grade
GOST 19281-2014Higher-strength rolled steelsLow-alloy strength grades and delivery rules
GOST 27772-2021Structural steel rolled productsS-series Russian construction specifications
GOST 5632-2014Stainless heat/corrosion-resistant alloy gradesRussian chemistry designations
GOST 5582-75Corrosion-resistant heat-resistant thin sheetStainless flat products
GOST 7350-77Corrosion-resistant thick plateStainless flat products
GOST 10704-91Straight-seam electric-welded tube dimensionsDimensions; companion technical requirements needed
GOST 10705-80ERW longitudinal carbon/low-alloy tube technical requirementsOD 10–630 mm per Rosstandart description
GOST 10706-76Large electric-welded straight-seam tubeHigher-diameter special route
GOST 8732-78Hot-deformed seamless tubes, dimensionsSeamless route
GOST 8734-75Cold-deformed seamless tubes, dimensionsSeamless route
GOST 8731-74 / 8733-74Seamless tube technical requirementsUsed alongside dimensions standards
GOST 9940-81Hot-deformed seamless corrosion-resistant tubesStainless tubes
GOST 9941-81Cold/warm-deformed seamless corrosion-resistant tubesStainless tubes
GOST 11068-81Electric-welded corrosion-resistant steel tubesStainless welded tubes
GOST 13663-86Profile steel tubes technical requirementsProfile tubes
GOST 9.315-91Hot-dip aluminum protective coating on fabricated productsExplicitly excludes continuously coated flat products
GOST 14918-2020Continuously coated zinc and zinc-alloy sheetContains Al–Zn coating, NOT equivalent to Al–Si aluminized steel
GOST R ISO 17925-2012Zinc/aluminium coating mass and chemistry test methodsTesting standard; not product specification
GOST 10692-2015Steel tube acceptance, marking, packing, shippingGeneral tube requirements

Carbon and mild steel grade families

DesignationTypical sourceCategoryImportant qualification
Ст0–Ст6 (St0–St6)GOST 380Ordinary-quality structural steelSuffix кп (rimmed), пс (semi-killed), сп (killed) when specified
Ст3сп / Ст3псGOST 380Common structural steelExact chemistry and mechanical class vary by product
08 / 08кп / 08псGOST 1050 / flat steel rulesVery-low-carbon forming steelQualitative comparison to SAE 1008; not direct equivalent
10 / 15 / 20GOST 1050Low-carbon engineering steelCommon tube/parts substrates; heat/condition matters
25 / 30 / 35GOST 1050Medium-carbon steelIncreasing strength and welding sensitivity
40 / 45 / 50GOST 1050Medium carbon heat-treatment steelsNot substitutes for deep-drawing DC grades
08Ю / 08кп / 08псGOST 9045 / 16523 product-dependentCold formingDrawing classes and delivery condition determine performance
09Г2СGOST 19281 and product-specificLow-alloy structural/weldable steelCommon structural and piping uses; validate applicable tube norm
10Г2 / 17Г1СProduct-specificMn-alloy grades for higher-strength applicationsCheck actual GOST grade listing and dimensions

Understanding Russian carbon steel notation

Numeric grades such as 08, 10 and 20 indicate approximate carbon level in hundredths of one percent in the Russian designation system, but actual permitted chemistry must be read from the applicable specification. Ст3сп identifies an ordinary-quality carbon steel and deoxidation state, not the same grading system as SAE 1010 or DC01. Quality, delivery, surface and drawing classifications are product-standard dependent.

Stainless steel GOST grade comparisons

Russian designationUS/EN screening referenceMetallurgical familyWhy verification is needed
08Х18Н10304 broad chemistry analogueCr–Ni austeniticDo not assume ASTM 304 identical: C and Ni boundaries differ
03Х18Н11304L family comparisonLow-C austeniticCheck nickel requirement and availability
12Х18Н10Т321 family comparisonTitanium-stabilized austeniticCarbon limits differ substantially from 321
08Х18Н10Т321 family comparisonTi-stabilized austeniticCheck exact melt analysis and tube norm
10Х17Н13М2Т316Ti family comparisonMo-bearing Ti-stabilizedNot identical to 316 / 316L
03Х17Н14М3316L/317L comparison onlyMo-bearing low-C austeniticHigher Mo/Ni may fall outside ASTM 316L
06ХН28МДТHigh-Ni acid-resistantSpecial chemical serviceNo casual 904L substitution
08Х13410S/low-C Cr13 comparisonLow-chromium ferritic/martensitic categoryHeat treatment influences properties
12Х13410 broad comparisonMartensitic Cr13Not 409
20Х13 / 30Х13 / 40Х13420 familiesMartensitic gradesDifferent carbon and hardness
12Х17430 broad comparisonFerritic Cr17Welding/formability and C limits must be verified
08Х17ТTi-stabilized ferritic broad comparison409/439 not guaranteedRequires Cr, Ti, C comparison
15Х25ТHigh-Cr ferriticHeat resistanceDifferent from 446 unless verified

How Russian alloy names are constructed

Examples: 12Х18Н10Т approximately indicates 0.12% C upper-level naming convention, 18% Cr, 10% Ni and titanium stabilization; Х means chromium, Н nickel, М molybdenum, Т titanium, Г manganese and Ю aluminum. The naming convention is not a substitute for the chemistry table. Transliteration of the Russian character Х as X or Kh can create misleading catalog entries.

Aluminized steel under GOST

No generic AS120 assumption

The widely cited GOST 14918-2020 covers hot-dip zinc and zinc-alloy coated sheet, including aluminum–zinc (АЦ) coatings. It is not a general equivalent of EN 10346 DX54D+AS120 or ASTM A463 Type 1 Al–Si coating. GOST 9.315-91 addresses hot-dip aluminum coatings on fabricated products, explicitly excluding continuously coated sheet. Accordingly, when a Russian buyer requests aluminum–silicon coated strip or tube, identify a specific applicable GOST/TU/STO or mutually accept EN 10346 or ASTM A463 with agreed testing; do not invent a GOST grade or coating code.

Product requestedPotential referenceTechnical decision
Bare low-carbon welded tubeGOST 10704 dimensions + GOST 10705 technical rulesCheck steel grade, supply class and test requirements
Bare stainless welded tubeGOST 11068 + GOST 5632Confirm exact Russian grade and chemical composition
Continuously Al–Si coated carbon stripNo blanket one-to-one GOST identifiedUse EN 10346 +AS or ASTM A463 by agreement, or verify an applicable TU
Al-coated fabricated carbon steel componentGOST 9.315-91Coating only; explicitly not coil-process standard
Al–Zn coated low-carbon sheetGOST 14918-2020Al–Zn is not Al–Si; do not quote as aluminized Type 1
409 stainless with Al–Si coatingGOST 5632 substrate only if correct grade exists, plus agreed coat specDual description and testing; no automatic GOST 409AL grade

300 series stainless grade register

AISI / tradeUNSEN screening cross-referenceMain tube relevanceIndicative chemistry, not acceptance limits
301S301001.4310 X10CrNi18-8austenitic; high work hardening; formed partsCr 16–18; Ni 6–8; C ≤0.15
302S302001.4319 (comparison only)austenitic; higher C than 304Cr 17–19; Ni 8–10; C ≤0.15
303S303001.4305 X8CrNiS18-9free-machining; sulfur; poor welding choiceCr 17–19; Ni 8–10; S ≥0.15
304S304001.4301 X5CrNi18-10general welded tube and fabricationCr 18–20; Ni 8–10.5; C ≤0.08
304LS304031.4307 / 1.4306lower carbon; welded assembliesCr 18–20; Ni 8–12; C ≤0.03
304HS304091.4948 (check product)elevated temperature; controlled carbonC 0.04–0.10; Cr 18–20; Ni 8–11
305S305001.4303 X4CrNi18-12deep forming; higher nickelCr 17–19; Ni 11–13
309SS309081.4833 X12CrNi23-13heat oxidation serviceCr 22–24; Ni 12–15; C ≤0.08
310SS310081.4845 X8CrNi25-21heat-resistant high chromium nickelCr 24–26; Ni 19–22; C ≤0.08
316S316001.4401 X5CrNiMo17-12-2molybdenum for chloride resistanceCr 16–18; Ni 10–14; Mo 2–3
316LS316031.4404 / 1.4432 / 1.4435welded chemical and hygienic tubesC ≤0.03; Cr 16–18; Mo 2–3
316TiS316351.4571 X6CrNiMoTi17-12-2Ti stabilized; hot serviceCr 16.5–18.5; Ni 10.5–13.5; Mo 2–2.5
317LS317031.4438 (comparison only)higher Mo; aggressive serviceCr 18–20; Ni 11–15; Mo 3–4
321S321001.4541 X6CrNiTi18-10Ti stabilized exhaust and heatCr 17–19; Ni 9–12; Ti controlled
347S347001.4550 X6CrNiNb18-10Nb stabilized weld/thermal applicationsCr 17–19; Ni 9–13; Nb controlled
904LN089041.4539 X1NiCrMoCu25-20-5high alloy austenitic; acid serviceCr 19–23; Ni 23–28; Mo 4–5; Cu 1–2

The chemistry column gives orientation ranges rounded from widely used specifications; acceptance requires the precise grade and edition’s chemical tables, product analysis tolerances and any agreed dual certification. EN variants under one US commercial name may have nonidentical nickel or molybdenum bounds.

400 series stainless grade register

AISI / tradeUNSEN screening cross-referenceMain tube relevanceIndicative chemistry, not acceptance limits
405S405001.4002 X6CrAl13Al-alloyed ferritic stainless; distinct from coated steelCr 11.5–14.5; Al 0.10–0.30
409S409001.4512 X2CrTi12Ti stabilized; exhaust componentsCr 10.5–11.75; C ≤0.08; Ti stabilization
409LS40910 / EN variant1.4512 comparisonlow-C exhaust; check grade-specific producer chemistryExact chemistry depends designation
410S410001.4006 X12Cr13martensitic; may be heat treatedCr 11.5–13.5; C ≤0.15
410SS410081.4000 X6Cr13low-C ferritic counterpartCr 11.5–13.5; C ≤0.08
420S420001.4021 / 1.4028 variantsmartensitic; wear/hardness applicationsCr 12–14; C varies materially
430S430001.4016 X6Cr1717% chromium; household/ductingCr 16–18; Ni not specified as alloy addition
430Tivaries1.4510/1.4520 comparison onlystabilized ferritic; specify exact designationCr ~16–18; Ti controlled
434S434001.4113 X6CrMo17-1Mo-bearing ferritic corrosion upgradeCr 16–18; Mo ~0.75–1.25
436S436001.4526 comparisonMo-bearing and stabilized exhaust optionCr 16–18; Mo ~0.75–1.25
439S430351.4510 X3CrTi17Ti stabilized; exhaust and exchangersCr 17–19; Ti controlled
441S43940 / S439321.4509 X2CrTiNb18dual stabilized Ti+Nb; elevated-temp exhaustCr ~17.5–18.5; Ti+Nb controlled
444S444001.4521 X2CrMoTi18-2Mo-bearing ferritic; high corrosion resistanceCr 17–20; Mo 1.75–2.5
446S446001.4749 comparisonhigh-Cr oxidation resistanceCr 23–27

The 400 series spans ferritic and martensitic alloys. 409, 430, 439, 441 and 444 are ferritic; 410 and many 420 variants are martensitic. They cannot be substituted by series number alone. Stabilization is essential to welding and heat-resistance performance.

Special study 409AL and aluminized stainless

Two different uses of a similar name

In exhaust purchasing, “409AL”, “409 Aluminized” or “aluminized 409” commonly describes a 409 ferritic stainless substrate with hot-dip Al–Si coating (often Type 1), supplied as coated strip under ASTM A463/A463M or an agreed equivalent manufacturing specification. In other metallurgical contexts “409Al” may designate an aluminum-stabilized ferritic alloy rather than a surface-coated product. The suffix AL is not a safe stand-alone specification or universally standardized UNS grade.

CheckRequired PO or MTC statement
SubstrateUNS S40900 / other explicitly specified 409 family grade; separate heat analysis
CoatingAl–Si Type 1 vs pure-Al Type 2; applicable sheet standard or mill technical specification
Coating massExact T1 / T1M or EN AS designation, total-both-sides vs per-side convention
Finished tubeTube standard, process (ERW, TIG/laser), OD, wall and length tolerances
WeldTreatment of weld seam and local coating loss; corrosion qualification if required
VerificationCoating mass/thickness; adhesion; substrate PMI; tube dimensional and leak tests

A 409 substrate with aluminized coating is neither plain aluminized carbon steel nor bare 409 stainless. The coating may be damaged or absent at the weld seam and cut ends; agree on treatment and service testing. The producer should specify coating condition after tube forming, not only before it.

GOST carbon steels practical composition sheets

GradeC % typical standard bandMn % typical bandSi % typical bandTechnical implication
080.05–0.120.25–0.500.17–0.37 (killed variant)Drawing, low-carbon welding
100.07–0.140.35–0.650.17–0.37Welded/engineered tube
150.12–0.190.35–0.650.17–0.37General purpose
200.17–0.240.35–0.650.17–0.37Common tube material
350.32–0.400.50–0.800.17–0.37Higher strength, less forming
450.42–0.500.50–0.800.17–0.37Machining/heat treatment

The numerical chemistry is for screening the GOST 1050 family only, with killed-steel Si where explicitly stated. The rimmed/semi-killed variants, permitted residuals, amendments and product-specific chemistry must be verified before MTC dual-certification. Strength values vary with section size and heat treatment and cannot be taken from a chemistry designation.

Individual GOST tube order decisions

08Х18Н10

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 304 broad chemistry analogue. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionCr–Ni austenitic; validate supplier anneal / heat treatment and surface state.
Tube production considerationsDo not assume ASTM 304 identical: C and Ni boundaries differ; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

03Х18Н11

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 304L family comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionLow-C austenitic; validate supplier anneal / heat treatment and surface state.
Tube production considerationsCheck nickel requirement and availability; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

12Х18Н10Т

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 321 family comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionTitanium-stabilized austenitic; validate supplier anneal / heat treatment and surface state.
Tube production considerationsCarbon limits differ substantially from 321; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

08Х18Н10Т

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 321 family comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionTi-stabilized austenitic; validate supplier anneal / heat treatment and surface state.
Tube production considerationsCheck exact melt analysis and tube norm; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

10Х17Н13М2Т

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 316Ti family comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionMo-bearing Ti-stabilized; validate supplier anneal / heat treatment and surface state.
Tube production considerationsNot identical to 316 / 316L; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

03Х17Н14М3

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 316L/317L comparison only. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionMo-bearing low-C austenitic; validate supplier anneal / heat treatment and surface state.
Tube production considerationsHigher Mo/Ni may fall outside ASTM 316L; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

06ХН28МДТ

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison High-Ni acid-resistant. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionSpecial chemical service; validate supplier anneal / heat treatment and surface state.
Tube production considerationsNo casual 904L substitution; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

08Х13

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 410S/low-C Cr13 comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionLow-chromium ferritic/martensitic category; validate supplier anneal / heat treatment and surface state.
Tube production considerationsHeat treatment influences properties; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

12Х13

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 410 broad comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionMartensitic Cr13; validate supplier anneal / heat treatment and surface state.
Tube production considerationsNot 409; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

20Х13 / 30Х13 / 40Х13

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 420 families. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionMartensitic grades; validate supplier anneal / heat treatment and surface state.
Tube production considerationsDifferent carbon and hardness; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

12Х17

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison 430 broad comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionFerritic Cr17; validate supplier anneal / heat treatment and surface state.
Tube production considerationsWelding/formability and C limits must be verified; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

08Х17Т

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison Ti-stabilized ferritic broad comparison. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical condition409/439 not guaranteed; validate supplier anneal / heat treatment and surface state.
Tube production considerationsRequires Cr, Ti, C comparison; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

15Х25Т

Specification fieldTechnical requirement / engineering guidance
Chemical compositionGrade chemistry defined by GOST 5632-2014; US screening comparison High-Cr ferritic. Obtain cast/product analysis of C, Cr, Ni, Mo and Ti/Nb where applicable.
Mechanical propertiesUse product-specific delivery and heat-treatment mechanical limits; GOST 5632 is primarily a grade/chemistry standard, not a universal tube yield/tensile standard.
Supply and metallurgical conditionHeat resistance; validate supplier anneal / heat treatment and surface state.
Tube production considerationsDifferent from 446 unless verified; distinguish welded tube per GOST 11068 from seamless tube per GOST 9940 or 9941.
Inspection, test and certificateHeat analysis, tube dimensions, tensile/flattening/flaring when specified, nondestructive/leak test, and documentation under applicable GOST tube product norm.
Basis / precisionGrade correspondence is screening only; no certified ASTM/EN equivalence without both-standard qualification.

Individual stainless steel technical specification sheets

301 stainless steel S30100

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Ni 6–8; C ≤0.15
Mechanical propertiesCold-worked tempers can increase strength greatly; annealed values must not be applied to half-hard/full-hard strip.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4310 X10CrNi18-8) and corrosion exposure.
Tube production considerationsStrong work hardening; control rolling and tube-forming strain.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

302 stainless steel S30200

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 8–10; C ≤0.15
Mechanical propertiesMechanical properties depend on annealed or cold-worked temper.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4319 (comparison only)) and corrosion exposure.
Tube production considerationsHigher carbon means evaluate weld sensitization.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

303 stainless steel S30300

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 8–10; S ≥0.15
Mechanical propertiesMechanical strength depends on product form and temper.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4305 X8CrNiS18-9) and corrosion exposure.
Tube production considerationsSulfur addition improves machinability but reduces fusion-weld suitability.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

304 stainless steel S30400

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 18–20; Ni 8–10.5; C ≤0.08
Mechanical propertiesTypical solution-annealed plate/sheet minimum: Rp0.2 ~205 MPa; Rm ~515 MPa; elongation ~40% under common ASTM flat-product conditions. These figures are NOT universal finished-tube limits.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4301 X5CrNi18-10) and corrosion exposure.
Tube production considerationsTIG/laser or qualified ERW; assess seam corrosion, ID bead, and sensitization.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

304L stainless steel S30403

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 18–20; Ni 8–12; C ≤0.03
Mechanical propertiesTypical annealed flat-product minima often Rp0.2 ~170 MPa, Rm ~485 MPa, A ~40%; verify actual product-standard edition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4307 / 1.4306) and corrosion exposure.
Tube production considerationsLow carbon preferred for welded parts; 304/304L dual certificate requires both chemistries and all mechanical requirements.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

304H stainless steel S30409

Specification fieldTechnical requirement / engineering guidance
Chemical compositionC 0.04–0.10; Cr 18–20; Ni 8–11
Mechanical propertiesHigh-temperature grades require carbon control and elevated-temperature design values.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4948 (check product)) and corrosion exposure.
Tube production considerationsNot interchangeable with 304L; confirm thermal service and heat treatment.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

305 stainless steel S30500

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 11–13
Mechanical propertiesCold-forming optimized; yield/tensile depend on condition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4303 X4CrNi18-12) and corrosion exposure.
Tube production considerationsExcellent deep formability; check availability of tube coil.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

309S stainless steel S30908

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 22–24; Ni 12–15; C ≤0.08
Mechanical propertiesHeat-resistant austenitic; strength is condition and temperature dependent.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4833 X12CrNi23-13) and corrosion exposure.
Tube production considerationsOxidation/thermal cycling design matters more than generic room-temperature strength.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

310S stainless steel S31008

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 24–26; Ni 19–22; C ≤0.08
Mechanical propertiesHeat-resistant austenitic; check high-temperature creep/oxidation rating separately.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4845 X8CrNi25-21) and corrosion exposure.
Tube production considerationsHigh alloy weld consumable and thermal expansion considerations.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

316 stainless steel S31600

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Ni 10–14; Mo 2–3
Mechanical propertiesCommon annealed flat-product minima: Rp0.2 ~205 MPa, Rm ~515 MPa, A ~40%; do not apply to every tube product.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4401 X5CrNiMo17-12-2) and corrosion exposure.
Tube production considerationsMo enhances pitting resistance; not immune to chloride stress corrosion.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

316L stainless steel S31603

Specification fieldTechnical requirement / engineering guidance
Chemical compositionC ≤0.03; Cr 16–18; Mo 2–3
Mechanical propertiesCommon annealed flat-product minima: Rp0.2 ~170 MPa, Rm ~485 MPa, A ~40%; verify product-specific requirements.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4404 / 1.4432 / 1.4435) and corrosion exposure.
Tube production considerationsLower carbon for welded corrosion service; surface passivation may be specified.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

316Ti stainless steel S31635

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16.5–18.5; Ni 10.5–13.5; Mo 2–2.5
Mechanical propertiesCondition, temperature and specimen direction determine applicable mechanical minima.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4571 X6CrNiMoTi17-12-2) and corrosion exposure.
Tube production considerationsTi stabilized; specify solution treatment and avoid assuming same chemistry as 316L.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

317L stainless steel S31703

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 18–20; Ni 11–15; Mo 3–4
Mechanical propertiesHigher Mo chemistry; mechanical values require exact product specification.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4438 (comparison only)) and corrosion exposure.
Tube production considerationsCorrosion qualification should match chloride/acidity environment.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

321 stainless steel S32100

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 9–12; Ti controlled
Mechanical propertiesCommon annealed flat-product tensile minimum around 515 MPa; full yield/elongation require edition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4541 X6CrNiTi18-10) and corrosion exposure.
Tube production considerationsTitanium stabilization and weld heat exposure make treatment critical.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

347 stainless steel S34700

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 9–13; Nb controlled
Mechanical propertiesStabilized Cr–Ni steel; property limits depend on standard and condition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4550 X6CrNiNb18-10) and corrosion exposure.
Tube production considerationsNb stabilization; specify temperature cycling, weld process and test plan.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

904L stainless steel N08904

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 19–23; Ni 23–28; Mo 4–5; Cu 1–2
Mechanical propertiesHigh alloy austenitic; minimum properties are product- and condition-specific.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4539 X1NiCrMoCu25-20-5) and corrosion exposure.
Tube production considerationsHigh Ni/Mo/Cu content; demanding weld qualification and PMI.
Inspection, test and certificateUse GOST 11068 / GOST 9940 / GOST 9941 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

405 stainless steel S40500

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 11.5–14.5; Al 0.10–0.30
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionAl-alloyed ferritic stainless; distinct from coated steel; match exact UNS and EN designation (1.4002 X6CrAl13), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

409 stainless steel S40900

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 10.5–11.75; C ≤0.08; Ti stabilization
Mechanical propertiesTypical annealed mechanical properties: yield roughly 170–240 MPa, tensile 380–480 MPa, elongation ~20–30%; commercial supplier typicals, not acceptance minima.
Supply and metallurgical conditionTi stabilized; exhaust components; match exact UNS and EN designation (1.4512 X2CrTi12), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

409L stainless steel S40910 / EN variant

Specification fieldTechnical requirement / engineering guidance
Chemical compositionExact chemistry depends designation
Mechanical propertiesLower interstitial chemistry; properties depend on exact UNS and strip anneal.
Supply and metallurgical conditionlow-C exhaust; check grade-specific producer chemistry; match exact UNS and EN designation (1.4512 comparison), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

410 stainless steel S41000

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 11.5–13.5; C ≤0.15
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionmartensitic; may be heat treated; match exact UNS and EN designation (1.4006 X12Cr13), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

410S stainless steel S41008

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 11.5–13.5; C ≤0.08
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionlow-C ferritic counterpart; match exact UNS and EN designation (1.4000 X6Cr13), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

420 stainless steel S42000

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 12–14; C varies materially
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionmartensitic; wear/hardness applications; match exact UNS and EN designation (1.4021 / 1.4028 variants), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

430 stainless steel S43000

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Ni not specified as alloy addition
Mechanical propertiesTypical annealed yield roughly 205–310 MPa, tensile ~450–550 MPa, elongation ~20–30%; supplier typicals, not acceptance minima.
Supply and metallurgical condition17% chromium; household/ducting; match exact UNS and EN designation (1.4016 X6Cr17), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

430Ti stainless steel varies

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr ~16–18; Ti controlled
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionstabilized ferritic; specify exact designation; match exact UNS and EN designation (1.4510/1.4520 comparison only), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

434 stainless steel S43400

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Mo ~0.75–1.25
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionMo-bearing ferritic corrosion upgrade; match exact UNS and EN designation (1.4113 X6CrMo17-1), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

436 stainless steel S43600

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Mo ~0.75–1.25
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionMo-bearing and stabilized exhaust option; match exact UNS and EN designation (1.4526 comparison), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

439 stainless steel S43035

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ti controlled
Mechanical propertiesTypical annealed yield ~240–320 MPa, tensile ~415–520 MPa; check actual strip MTC.
Supply and metallurgical conditionTi stabilized; exhaust and exchangers; match exact UNS and EN designation (1.4510 X3CrTi17), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

441 stainless steel S43940 / S43932

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr ~17.5–18.5; Ti+Nb controlled
Mechanical propertiesTypical annealed yield ~250–350 MPa, tensile ~430–550 MPa; check grade variant and coil certificate.
Supply and metallurgical conditiondual stabilized Ti+Nb; elevated-temp exhaust; match exact UNS and EN designation (1.4509 X2CrTiNb18), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

444 stainless steel S44400

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–20; Mo 1.75–2.5
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionMo-bearing ferritic; high corrosion resistance; match exact UNS and EN designation (1.4521 X2CrMoTi18-2), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

446 stainless steel S44600

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 23–27
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionhigh-Cr oxidation resistance; match exact UNS and EN designation (1.4749 comparison), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to GOST 11068 / GOST 9940 / GOST 9941 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

Tube purchase-order specification matrix

FieldWhat an engineering inquiry or PO must state
ProductWelded round tube; intended mechanical, exhaust, heat-exchanger or pressure duty
Base gradeExact material designation and source sheet/strip standard + edition
CoatingNone / Al–Si / Al / Zn–Al; mass, type, both-face convention, coil condition
Tube standardApplicable finished-product norm and edition; do not infer from strip grade
DimensionsOD x nominal wall x cut length; tolerances, eccentricity, straightness, ovality
ProductionHF-ERW / laser / TIG; weld-bead treatment; anneal/pickling/passivation if relevant
VerificationChemistry, tensile or hardness, flattening/flaring/bend, leak/eddy/UT where applicable
CertificationEN 10204 3.1 or other agreed inspection certificate; heat/coil/tube traceability
PackingBlue-wrapped bundles, without pallet/sleeve/slings if requested; moisture protection

Tube manufacturing and acceptance checks

Coil receipt

Record heat number, coil number, coating face/mass, thickness, tensile condition and supplier MTC. A tube made from a compliant coil is not automatically a compliant tube.

Slitting and forming

Confirm strip edge condition, strip width, springback, seam orientation, and coating crack tolerance. High-strength sheet may have limited formability.

Weld process

Identify HF-ERW, TIG or laser; assess weld speed and heat input, seam bead and heat-affected region. High-Cr ferritic tubes need controlled welding and may require post-weld treatment.

Dimensional checks

Measure OD, nominal and minimum wall, out-of-roundness, length, straightness, end squareness and bend/ovality where specified. Use the actual tube standard tolerances.

Nondestructive/leak testing

Apply the specific test prescribed or agreed for the product: eddy-current, ultrasonic, pneumatic or hydrostatic. An inspection technology is not a substitute for the required acceptance level.

Marking and documentation

Record manufacturer, standard, grade, size, batch/heat and inspection results. Any claim to ASTM, EN or GOST should be supported by all relevant mandatory tests.

Example Russian procurement descriptions

Труба стальная электросварная прямошовная, размеры по ГОСТ 10704-91, технические требования по ГОСТ 10705-80, марка стали 20 по применимому стандарту, Ø101,6 x 2,0 x 5840 мм, категория поставки и испытания по договору.

Труба электросварная из коррозионно-стойкой стали по ГОСТ 11068-81, марка 08Х18Н10 (при подтверждении применимости), Ø114,3 x 1,5 x 1198 мм, требования к контролю и документам по заказу.

Труба из алюминированной полосы DX54D+AS120 по EN 10346 (стандарт основы/покрытия согласован сторонами), изготовление трубы по согласованному техническому заданию; подтверждение покрытия в зоне сварного шва обязательно.

Russian standards and source links

https://protect.gost.ru/gost/details/d6ac3954-d07e-4a10-a038-f3ab9b1d5b7b

https://protect.gost.ru/gost/details/866e7dab-a11a-44fe-8d98-eed7fa4f2b7b

https://protect.gost.ru/gost/details/176e3435-29c7-4891-9217-afcf4ae3f16d

https://protect.gost.ru/gost/details/ea2413bd-eb14-49fd-8df4-078b6a698a02

https://protect.gost.ru/gost/details/3a1e2068-2573-4b89-928f-1f524540d946

https://protect.gost.ru/gost/details/84bf5d63-0bbe-4ad6-b267-9162f7ce6cb8

Back to Insights

Scan the code to connect.