Purpose and interpretation

This guide connects raw-material/coil designations with specifications for finished tubes. A grade alone does not define a compliant tube: the purchase order must also identify product form, applicable edition, dimensions, tolerance class, delivery condition, testing, inspection and documentation. Tables are curated commercial grade families, not a reproduction of copyrighted standards or an assertion that every grade ever standardized is included.

Important conformity principle

A comparison such as ASTM 304 ≈ EN 1.4301 ≈ a GOST chromium–nickel grade is a screening aid only. Chemical limits, deoxidation, stabilization, mechanical requirements, permitted processes, heat treatment and tests can differ. Never print an untested alternative standard on an MTC, and never treat a flat-sheet standard as finished-tube certification.

Standards register and applicability

StandardApplies toCommercial interpretation
ASTM A1008/A1008MCold-rolled uncoated carbon and HSLA sheetRaw strip: CS, DS, DDS, EDDS, SS and HSLA families
ASTM A1011/A1011MHot-rolled carbon/structural/HSLA sheet and stripRaw strip: CS, DS, SS grades, HSLA; thickness dependent
ASTM A568/A568MGeneral requirements for steel sheet, carbon and HSLASheet ordering, tolerances, common requirements
ASTM A463/A463MContinuously hot-dip aluminum-coated steel sheetType 1 Al–Si and Type 2 Al; coating & base steel grades
ASTM A924/A924MGeneral requirements for metallic-coated sheetReferenced requirements and dimensions for coated sheet
ASTM A240/A240MCr and Cr–Ni stainless flat productsSheet/strip for 300/400 stainless substrates
ASTM A480/A480MGeneral requirements for stainless flat productsDimensions, finish and ordering requirements
ASTM A513/A513MERW carbon and alloy mechanical tubingCommon mechanical/exhaust tube route; type/grade must be stated
ASTM A500/A500MStructural carbon tube, round or shapedLoad-bearing welded or seamless structural tubing
ASTM A53/A53MBlack or hot-dip zinc-coated welded/seamless steel pipeConveyance/ordinary piping; Grade A/B
ASTM A106/A106MSeamless carbon-steel pipe for high-temperature servicePressure/piping route; not generic ERW tube
ASTM A178/A178MERW carbon and carbon-manganese boiler tubesThermal duty and mandatory tests
ASTM A214/A214MERW carbon steel heat-exchanger/condenser tubesHeat-transfer equipment
ASTM A249/A249MWelded austenitic boiler and exchanger tubes300-series thermal tubes; process/testing controlled
ASTM A269/A269MSeamless/welded austenitic general service tubing300-series tubing
ASTM A268/A268MSeamless/welded ferritic and martensitic tubing400-series tubing; verify specific grade listing
ASTM A554Welded stainless mechanical tubingMechanical/decorative 300 and 400 series
ASTM A270/A270MSeamless/welded austenitic sanitary tubingFood/pharmaceutical sanitary requirements
ASTM A312/A312MSeamless/welded austenitic stainless pipeProcess piping rather than mechanical tube
ASTM A1016/A1016MGeneral requirements for steel tube groupsReferenced supplementary testing/inspection
SAE J403 / J404Carbon / alloy-steel chemistry designation systemsExamples 1008, 1010, 1018, 1020, 1045; not tube standards

Carbon steel and mild steel families

Grade/familyCharacterTypical useKey qualification
SAE 1006 / 1008Very low carbonCommercial forming, thin-wall tube; chemistry grade
SAE 1010 / 1012Low carbonWeldable mechanical tubes; grade identity via SAE J403
SAE 1015 / 1018 / 1020Low-to-medium carbonGeneral engineering; higher C limits cold-forming vs 1008
SAE 1022 / 1026Higher carbon mechanical tubing feedstockCommon A513 mechanical tube options subject to process
SAE 1040 / 1045Medium carbonStrength/machining and heat treatment; greater welding controls
ASTM A1008 CS Type A/B/CCold-rolled commercial sheetCommercial forming; chemistry and test limits grade dependent
ASTM A1008 DS/DDS/EDDSCold-rolled drawing familiesDeep drawing; no one-to-one DC01 to DC06 equivalence
ASTM A1008 SS 25–60Cold-rolled structural sheetGrade numerals denote yield strength in ksi, with type distinctions
ASTM A1011 SS 30–70Hot-rolled structural sheetMechanical grade; availability depends edition/thickness
ASTM A1011 HSLAS 45–80Hot-rolled HSLA familiesHigh strength and weight reduction; verify formability
ASTM A36Structural carbon plate/shapesNot a universal tube-coil or tube standard
ASTM A500 Grade B/C/DStructural hollow sectionsFinal tube grade with specified mechanical properties
ASTM A53 Grade A/BPipe gradePipe pressure/hydro requirements, not equivalent to A513

Why DC01 is not an American grade

DC01 belongs to EN 10130. US cold-rolled commercial/drawing steel is ordered through ASTM A1008/A1008M CS/DS/DDS/EDDS (or to a qualified SAE chemistry where specified). A US CS grade is not certified to DC01 unless tested and documented to both standards; tensile, yield, elongation and surface/aging requirements must all be reviewed.

Aluminized steel and coating options

ASTM A463 designationType / roleTechnical or ordering consideration
CS Type A, B, CCommercial formingType 1 or Type 2 coating per grade and order
FSForming SteelImproved formability; verify edition availability
DDSDeep Drawing SteelMore severe draw operations
EDDSExtra Deep Drawing SteelVery demanding drawing; supplier availability
SS Grades 33, 37, 40, 50 etc.StructuralExact grade/class permitted by edition
HSLAS Type A and BHigh-strength low-alloyGrade strength and class per specification
FSS 409 and 439Ferritic stainless substrateCoated stainless option: distinct from coated carbon
T1-13 / T1-20 / T1-25 / T1-40 / T1-60Type 1 coating mass in oz/ft², both sidesConfirm available designation/edition; T1-40 ≈ 122 g/m²
T1M 40 / 60 / 75 / 100 / 120 / 150 etc.Type 1 metric coating massMass in g/m² combined both sides; confirm listed designation
T2-100Type 2 predominantly aluminum coatingDifferent purpose, adhesion and appearance; no silent switch

Type 1 is an aluminum–silicon alloy coating intended for oxidation and heat resistance. Type 2 is substantially pure aluminum and differs in coating properties. ASTM Type 1 T1-40 uses approximately 0.40 oz/ft² total both faces, equivalent to approximately 122 g/m²; EN AS120 is near it by coating mass, not automatic full equivalence. Numeric coating values are mass, not minimum local thickness.

300 series stainless grade register

AISI / tradeUNSEN screening cross-referenceMain tube relevanceIndicative chemistry, not acceptance limits
301S301001.4310 X10CrNi18-8austenitic; high work hardening; formed partsCr 16–18; Ni 6–8; C ≤0.15
302S302001.4319 (comparison only)austenitic; higher C than 304Cr 17–19; Ni 8–10; C ≤0.15
303S303001.4305 X8CrNiS18-9free-machining; sulfur; poor welding choiceCr 17–19; Ni 8–10; S ≥0.15
304S304001.4301 X5CrNi18-10general welded tube and fabricationCr 18–20; Ni 8–10.5; C ≤0.08
304LS304031.4307 / 1.4306lower carbon; welded assembliesCr 18–20; Ni 8–12; C ≤0.03
304HS304091.4948 (check product)elevated temperature; controlled carbonC 0.04–0.10; Cr 18–20; Ni 8–11
305S305001.4303 X4CrNi18-12deep forming; higher nickelCr 17–19; Ni 11–13
309SS309081.4833 X12CrNi23-13heat oxidation serviceCr 22–24; Ni 12–15; C ≤0.08
310SS310081.4845 X8CrNi25-21heat-resistant high chromium nickelCr 24–26; Ni 19–22; C ≤0.08
316S316001.4401 X5CrNiMo17-12-2molybdenum for chloride resistanceCr 16–18; Ni 10–14; Mo 2–3
316LS316031.4404 / 1.4432 / 1.4435welded chemical and hygienic tubesC ≤0.03; Cr 16–18; Mo 2–3
316TiS316351.4571 X6CrNiMoTi17-12-2Ti stabilized; hot serviceCr 16.5–18.5; Ni 10.5–13.5; Mo 2–2.5
317LS317031.4438 (comparison only)higher Mo; aggressive serviceCr 18–20; Ni 11–15; Mo 3–4
321S321001.4541 X6CrNiTi18-10Ti stabilized exhaust and heatCr 17–19; Ni 9–12; Ti controlled
347S347001.4550 X6CrNiNb18-10Nb stabilized weld/thermal applicationsCr 17–19; Ni 9–13; Nb controlled
904LN089041.4539 X1NiCrMoCu25-20-5high alloy austenitic; acid serviceCr 19–23; Ni 23–28; Mo 4–5; Cu 1–2

The chemistry column gives orientation ranges rounded from widely used specifications; acceptance requires the precise grade and edition’s chemical tables, product analysis tolerances and any agreed dual certification. EN variants under one US commercial name may have nonidentical nickel or molybdenum bounds.

400 series stainless grade register

AISI / tradeUNSEN screening cross-referenceMain tube relevanceIndicative chemistry, not acceptance limits
405S405001.4002 X6CrAl13Al-alloyed ferritic stainless; distinct from coated steelCr 11.5–14.5; Al 0.10–0.30
409S409001.4512 X2CrTi12Ti stabilized; exhaust componentsCr 10.5–11.75; C ≤0.08; Ti stabilization
409LS40910 / EN variant1.4512 comparisonlow-C exhaust; check grade-specific producer chemistryExact chemistry depends designation
410S410001.4006 X12Cr13martensitic; may be heat treatedCr 11.5–13.5; C ≤0.15
410SS410081.4000 X6Cr13low-C ferritic counterpartCr 11.5–13.5; C ≤0.08
420S420001.4021 / 1.4028 variantsmartensitic; wear/hardness applicationsCr 12–14; C varies materially
430S430001.4016 X6Cr1717% chromium; household/ductingCr 16–18; Ni not specified as alloy addition
430Tivaries1.4510/1.4520 comparison onlystabilized ferritic; specify exact designationCr ~16–18; Ti controlled
434S434001.4113 X6CrMo17-1Mo-bearing ferritic corrosion upgradeCr 16–18; Mo ~0.75–1.25
436S436001.4526 comparisonMo-bearing and stabilized exhaust optionCr 16–18; Mo ~0.75–1.25
439S430351.4510 X3CrTi17Ti stabilized; exhaust and exchangersCr 17–19; Ti controlled
441S43940 / S439321.4509 X2CrTiNb18dual stabilized Ti+Nb; elevated-temp exhaustCr ~17.5–18.5; Ti+Nb controlled
444S444001.4521 X2CrMoTi18-2Mo-bearing ferritic; high corrosion resistanceCr 17–20; Mo 1.75–2.5
446S446001.4749 comparisonhigh-Cr oxidation resistanceCr 23–27

The 400 series spans ferritic and martensitic alloys. 409, 430, 439, 441 and 444 are ferritic; 410 and many 420 variants are martensitic. They cannot be substituted by series number alone. Stabilization is essential to welding and heat-resistance performance.

Special study 409AL and aluminized stainless

Two different uses of a similar name

In exhaust purchasing, “409AL”, “409 Aluminized” or “aluminized 409” commonly describes a 409 ferritic stainless substrate with hot-dip Al–Si coating (often Type 1), supplied as coated strip under ASTM A463/A463M or an agreed equivalent manufacturing specification. In other metallurgical contexts “409Al” may designate an aluminum-stabilized ferritic alloy rather than a surface-coated product. The suffix AL is not a safe stand-alone specification or universally standardized UNS grade.

CheckRequired PO or MTC statement
SubstrateUNS S40900 / other explicitly specified 409 family grade; separate heat analysis
CoatingAl–Si Type 1 vs pure-Al Type 2; applicable sheet standard or mill technical specification
Coating massExact T1 / T1M or EN AS designation, total-both-sides vs per-side convention
Finished tubeTube standard, process (ERW, TIG/laser), OD, wall and length tolerances
WeldTreatment of weld seam and local coating loss; corrosion qualification if required
VerificationCoating mass/thickness; adhesion; substrate PMI; tube dimensional and leak tests

A 409 substrate with aluminized coating is neither plain aluminized carbon steel nor bare 409 stainless. The coating may be damaged or absent at the weld seam and cut ends; agree on treatment and service testing. The producer should specify coating condition after tube forming, not only before it.

SAE carbon steel composition engineering cards

GradeNominal C %Nominal Mn %Material behaviorQuotation caveat
1006≤0.080.25–0.40Very soft / formingExact limits per SAE J403
1008≤0.100.30–0.50Cold formability and ERWExact grade/heat chemistry
10100.08–0.130.30–0.60Weldable tube feedstockConfirm residual elements
10150.13–0.180.30–0.60General purpose low-carbonTemper and process matter
10180.15–0.200.60–0.90Machining and tube stockForming more limited
10200.18–0.230.30–0.60Low-carbon engineeringMechanical properties by tube norm
10260.22–0.280.60–0.90Stronger mechanical tube stockWeld requirements greater
10450.43–0.500.60–0.90Heat-treatable medium carbonAvoid unspecific ERW claim

Composition bands are practical SAE J403 screening values, not an authoritative quotation of a specified revision. SAE 1008 and 1010 may have multiple industry chemistry practices. The finished tube performance changes strongly with ERW, DOM, cold work and heat treatment.

ASTM A463 aluminized coating mass detailed comparison

US designationCoating familyTotal both-face coating mass minimumApproximate metric equivalent
T1-13Type 1 Al–Si0.13 oz/ft²40 g/m²
T1-25Type 1 Al–Si0.25 oz/ft²76 g/m²
T1-40Type 1 Al–Si0.40 oz/ft²122 g/m²
T1-60Type 1 Al–Si0.60 oz/ft²183 g/m²
T1M 40Type 1 Al–Si40 g/m²~0.13 oz/ft²
T1M 120Type 1 Al–Si120 g/m²~0.39 oz/ft²

1 oz/ft² ≈ 305.15 g/m². Coating designation mass convention, sampling and minimum single-spot requirements must be checked in ASTM A463/A463M edition. Manufacturer data: Cleveland-Cliffs Aluminized Type 1 Product Data (2025). Type 1 typically contains about 9–11% silicon in the aluminum coating alloy.

US product mechanical requirements are not interchangeable

SpecificationRepresentative minimum yieldRepresentative minimum tensileWhat changes the result
A500 Grade B round structural tube~290 MPa~400 MPaEdition, shape/grade and heat treatment
A500 Grade C structural tube~345 MPa~425 MPaProduct specification, shape, edition
A53 Grade B pipe~240 MPa~415 MPaPipe grade and process
A513 mechanical tubenot a single grade-wide valuenot a single grade-wide valueSAE chemistry, type, as-welded/DOM/annealed
A554 stainless mechanicalgrade-specific / often order-agreedgrade-specific / often order-agreedAlloy, temper, finish and purchaser requirements

Individual stainless steel technical specification sheets

301 stainless steel S30100

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Ni 6–8; C ≤0.15
Mechanical propertiesCold-worked tempers can increase strength greatly; annealed values must not be applied to half-hard/full-hard strip.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4310 X10CrNi18-8) and corrosion exposure.
Tube production considerationsStrong work hardening; control rolling and tube-forming strain.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

302 stainless steel S30200

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 8–10; C ≤0.15
Mechanical propertiesMechanical properties depend on annealed or cold-worked temper.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4319 (comparison only)) and corrosion exposure.
Tube production considerationsHigher carbon means evaluate weld sensitization.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

303 stainless steel S30300

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 8–10; S ≥0.15
Mechanical propertiesMechanical strength depends on product form and temper.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4305 X8CrNiS18-9) and corrosion exposure.
Tube production considerationsSulfur addition improves machinability but reduces fusion-weld suitability.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

304 stainless steel S30400

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 18–20; Ni 8–10.5; C ≤0.08
Mechanical propertiesTypical solution-annealed plate/sheet minimum: Rp0.2 ~205 MPa; Rm ~515 MPa; elongation ~40% under common ASTM flat-product conditions. These figures are NOT universal finished-tube limits.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4301 X5CrNi18-10) and corrosion exposure.
Tube production considerationsTIG/laser or qualified ERW; assess seam corrosion, ID bead, and sensitization.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

304L stainless steel S30403

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 18–20; Ni 8–12; C ≤0.03
Mechanical propertiesTypical annealed flat-product minima often Rp0.2 ~170 MPa, Rm ~485 MPa, A ~40%; verify actual product-standard edition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4307 / 1.4306) and corrosion exposure.
Tube production considerationsLow carbon preferred for welded parts; 304/304L dual certificate requires both chemistries and all mechanical requirements.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

304H stainless steel S30409

Specification fieldTechnical requirement / engineering guidance
Chemical compositionC 0.04–0.10; Cr 18–20; Ni 8–11
Mechanical propertiesHigh-temperature grades require carbon control and elevated-temperature design values.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4948 (check product)) and corrosion exposure.
Tube production considerationsNot interchangeable with 304L; confirm thermal service and heat treatment.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

305 stainless steel S30500

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 11–13
Mechanical propertiesCold-forming optimized; yield/tensile depend on condition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4303 X4CrNi18-12) and corrosion exposure.
Tube production considerationsExcellent deep formability; check availability of tube coil.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

309S stainless steel S30908

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 22–24; Ni 12–15; C ≤0.08
Mechanical propertiesHeat-resistant austenitic; strength is condition and temperature dependent.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4833 X12CrNi23-13) and corrosion exposure.
Tube production considerationsOxidation/thermal cycling design matters more than generic room-temperature strength.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

310S stainless steel S31008

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 24–26; Ni 19–22; C ≤0.08
Mechanical propertiesHeat-resistant austenitic; check high-temperature creep/oxidation rating separately.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4845 X8CrNi25-21) and corrosion exposure.
Tube production considerationsHigh alloy weld consumable and thermal expansion considerations.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

316 stainless steel S31600

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Ni 10–14; Mo 2–3
Mechanical propertiesCommon annealed flat-product minima: Rp0.2 ~205 MPa, Rm ~515 MPa, A ~40%; do not apply to every tube product.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4401 X5CrNiMo17-12-2) and corrosion exposure.
Tube production considerationsMo enhances pitting resistance; not immune to chloride stress corrosion.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

316L stainless steel S31603

Specification fieldTechnical requirement / engineering guidance
Chemical compositionC ≤0.03; Cr 16–18; Mo 2–3
Mechanical propertiesCommon annealed flat-product minima: Rp0.2 ~170 MPa, Rm ~485 MPa, A ~40%; verify product-specific requirements.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4404 / 1.4432 / 1.4435) and corrosion exposure.
Tube production considerationsLower carbon for welded corrosion service; surface passivation may be specified.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

316Ti stainless steel S31635

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16.5–18.5; Ni 10.5–13.5; Mo 2–2.5
Mechanical propertiesCondition, temperature and specimen direction determine applicable mechanical minima.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4571 X6CrNiMoTi17-12-2) and corrosion exposure.
Tube production considerationsTi stabilized; specify solution treatment and avoid assuming same chemistry as 316L.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

317L stainless steel S31703

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 18–20; Ni 11–15; Mo 3–4
Mechanical propertiesHigher Mo chemistry; mechanical values require exact product specification.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4438 (comparison only)) and corrosion exposure.
Tube production considerationsCorrosion qualification should match chloride/acidity environment.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

321 stainless steel S32100

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 9–12; Ti controlled
Mechanical propertiesCommon annealed flat-product tensile minimum around 515 MPa; full yield/elongation require edition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4541 X6CrNiTi18-10) and corrosion exposure.
Tube production considerationsTitanium stabilization and weld heat exposure make treatment critical.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

347 stainless steel S34700

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ni 9–13; Nb controlled
Mechanical propertiesStabilized Cr–Ni steel; property limits depend on standard and condition.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4550 X6CrNiNb18-10) and corrosion exposure.
Tube production considerationsNb stabilization; specify temperature cycling, weld process and test plan.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

904L stainless steel N08904

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 19–23; Ni 23–28; Mo 4–5; Cu 1–2
Mechanical propertiesHigh alloy austenitic; minimum properties are product- and condition-specific.
Supply and metallurgical conditionAustenitic; confirm solution-annealed vs cold-worked temper, surface finish, EN number (1.4539 X1NiCrMoCu25-20-5) and corrosion exposure.
Tube production considerationsHigh Ni/Mo/Cu content; demanding weld qualification and PMI.
Inspection, test and certificateUse ASTM A554 / A269 / A268 as applicable tube-product specification matching application. Test chemistry/PMI, tensile as applicable, dimensions, weld integrity, surface and corrosion requirements; MTC to state grade, heat and precise standard edition.
Basis / precisionIndicative chemistry, not a complete mandatory heat/product analysis; strength examples refer to selected annealed flat products and require standard verification.

405 stainless steel S40500

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 11.5–14.5; Al 0.10–0.30
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionAl-alloyed ferritic stainless; distinct from coated steel; match exact UNS and EN designation (1.4002 X6CrAl13), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

409 stainless steel S40900

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 10.5–11.75; C ≤0.08; Ti stabilization
Mechanical propertiesTypical annealed mechanical properties: yield roughly 170–240 MPa, tensile 380–480 MPa, elongation ~20–30%; commercial supplier typicals, not acceptance minima.
Supply and metallurgical conditionTi stabilized; exhaust components; match exact UNS and EN designation (1.4512 X2CrTi12), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

409L stainless steel S40910 / EN variant

Specification fieldTechnical requirement / engineering guidance
Chemical compositionExact chemistry depends designation
Mechanical propertiesLower interstitial chemistry; properties depend on exact UNS and strip anneal.
Supply and metallurgical conditionlow-C exhaust; check grade-specific producer chemistry; match exact UNS and EN designation (1.4512 comparison), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

410 stainless steel S41000

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 11.5–13.5; C ≤0.15
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionmartensitic; may be heat treated; match exact UNS and EN designation (1.4006 X12Cr13), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

410S stainless steel S41008

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 11.5–13.5; C ≤0.08
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionlow-C ferritic counterpart; match exact UNS and EN designation (1.4000 X6Cr13), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

420 stainless steel S42000

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 12–14; C varies materially
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionmartensitic; wear/hardness applications; match exact UNS and EN designation (1.4021 / 1.4028 variants), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

430 stainless steel S43000

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Ni not specified as alloy addition
Mechanical propertiesTypical annealed yield roughly 205–310 MPa, tensile ~450–550 MPa, elongation ~20–30%; supplier typicals, not acceptance minima.
Supply and metallurgical condition17% chromium; household/ducting; match exact UNS and EN designation (1.4016 X6Cr17), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

430Ti stainless steel varies

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr ~16–18; Ti controlled
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionstabilized ferritic; specify exact designation; match exact UNS and EN designation (1.4510/1.4520 comparison only), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

434 stainless steel S43400

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Mo ~0.75–1.25
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionMo-bearing ferritic corrosion upgrade; match exact UNS and EN designation (1.4113 X6CrMo17-1), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

436 stainless steel S43600

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 16–18; Mo ~0.75–1.25
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionMo-bearing and stabilized exhaust option; match exact UNS and EN designation (1.4526 comparison), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

439 stainless steel S43035

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–19; Ti controlled
Mechanical propertiesTypical annealed yield ~240–320 MPa, tensile ~415–520 MPa; check actual strip MTC.
Supply and metallurgical conditionTi stabilized; exhaust and exchangers; match exact UNS and EN designation (1.4510 X3CrTi17), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

441 stainless steel S43940 / S43932

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr ~17.5–18.5; Ti+Nb controlled
Mechanical propertiesTypical annealed yield ~250–350 MPa, tensile ~430–550 MPa; check grade variant and coil certificate.
Supply and metallurgical conditiondual stabilized Ti+Nb; elevated-temp exhaust; match exact UNS and EN designation (1.4509 X2CrTiNb18), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

444 stainless steel S44400

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 17–20; Mo 1.75–2.5
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionMo-bearing ferritic; high corrosion resistance; match exact UNS and EN designation (1.4521 X2CrMoTi18-2), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

446 stainless steel S44600

Specification fieldTechnical requirement / engineering guidance
Chemical compositionCr 23–27
Mechanical propertiesMechanical requirements must be selected from the correct stainless flat or tube product standard and heat-treatment condition; no generic 400-series minimum applies.
Supply and metallurgical conditionhigh-Cr oxidation resistance; match exact UNS and EN designation (1.4749 comparison), anneal/temper, surface finish and stabilization.
Tube production considerationsFerritic alloys require attention to weld heat-affected-zone toughness, stabilizers and bead finish; martensitic grades may require heat treatment and hardness control.
Inspection, test and certificateOrder to ASTM A554 / A269 / A268 as applicable applicable tube norm; chemical analysis, dimensional checks, hardness/tensile where required, weld NDT or leak test, traceability and coating inspection if aluminized.
Basis / precisionChemistry overview and indicative industry property bands; exact pass/fail limits reside in the named edition and product form.

Tube purchase-order specification matrix

FieldWhat an engineering inquiry or PO must state
ProductWelded round tube; intended mechanical, exhaust, heat-exchanger or pressure duty
Base gradeExact material designation and source sheet/strip standard + edition
CoatingNone / Al–Si / Al / Zn–Al; mass, type, both-face convention, coil condition
Tube standardApplicable finished-product norm and edition; do not infer from strip grade
DimensionsOD x nominal wall x cut length; tolerances, eccentricity, straightness, ovality
ProductionHF-ERW / laser / TIG; weld-bead treatment; anneal/pickling/passivation if relevant
VerificationChemistry, tensile or hardness, flattening/flaring/bend, leak/eddy/UT where applicable
CertificationEN 10204 3.1 or other agreed inspection certificate; heat/coil/tube traceability
PackingBlue-wrapped bundles, without pallet/sleeve/slings if requested; moisture protection

Tube manufacturing and acceptance checks

Coil receipt

Record heat number, coil number, coating face/mass, thickness, tensile condition and supplier MTC. A tube made from a compliant coil is not automatically a compliant tube.

Slitting and forming

Confirm strip edge condition, strip width, springback, seam orientation, and coating crack tolerance. High-strength sheet may have limited formability.

Weld process

Identify HF-ERW, TIG or laser; assess weld speed and heat input, seam bead and heat-affected region. High-Cr ferritic tubes need controlled welding and may require post-weld treatment.

Dimensional checks

Measure OD, nominal and minimum wall, out-of-roundness, length, straightness, end squareness and bend/ovality where specified. Use the actual tube standard tolerances.

Nondestructive/leak testing

Apply the specific test prescribed or agreed for the product: eddy-current, ultrasonic, pneumatic or hydrostatic. An inspection technology is not a substitute for the required acceptance level.

Marking and documentation

Record manufacturer, standard, grade, size, batch/heat and inspection results. Any claim to ASTM, EN or GOST should be supported by all relevant mandatory tests.

Example ASTM purchase descriptions

ERW mechanical carbon tube, ASTM A513/A513M [edition], Type [ ], steel grade [SAE 1010 or agreed], OD 101.6 x WT 1.5 x L 3000 mm, condition [ ], dimensional tolerances [ ], eddy-current and MTC as agreed.

Aluminized exhaust tube, ASTM A463/A463M [edition] Type 1 CS Type B T1M 120 coil, formed into ERW tube to customer tube drawing / agreed tube product standard, OD 127 x WT 1.5 x L 5800 mm, welded-seam coating condition and bend test specified.

Welded stainless mechanical tube, ASTM A554 [edition], UNS S30400, OD 114.3 x WT 1.5 x L 1198 mm, finish and bead conditions agreed; ASTM A240 sheet certificate supplied additionally when required.

Aluminized 409 exhaust tube: ASTM A463 Type 1 FSS 409 substrate (confirm edition and exact UNS) with coating designation [ ], finished-tube requirements [ ]; separate substrate and coating test reports.

US references and verification links

https://store.astm.org/products-services/standards-and-publications/standards/steel-standards.html

https://store.astm.org/a0554-26.html

https://store.astm.org/standards/a513

https://northamerica.arcelormittal.com/products/flat-products/aluminized

https://d1io3yog0oux5.cloudfront.net/_eb4a0ea81b9379a33494f0f08bbd9931/clevelandcliffs/db/1190/10427/file/CLF_ProductData_AluminizedType1_032025.pdf

https://worldstainless.org/wp-content/uploads/2025/02/Module_05_Corrosion_Resistance_of_Stainless_Steels_en.pdf

https://nks.com/409-aluminized-stainless-steel-pdf/

Back to Insights

Scan the code to connect.