Shaped for Precision. Built for Industry.

Materials Standards

Chinese GB Steel Material Standards

National grade and coil specifications for carbon steel mild steel aluminized and stainless tube feedstock

Technical procurement and manufacturing reference | 17 November 2026 | Units: mm, MPa, mass % unless stated otherwise

Purpose and interpretation

This guide connects raw-material/coil designations with specifications for finished tubes. A grade alone does not define a compliant tube: the purchase order must also identify product form, applicable edition, dimensions, tolerance class, delivery condition, testing, inspection and documentation. Tables are curated commercial grade families, not a reproduction of copyrighted standards or an assertion that every grade ever standardized is included.

Important conformity principle

A comparison such as ASTM 304 ≈ EN 1.4301 ≈ a GOST chromium–nickel grade is a screening aid only. Chemical limits, deoxidation, stabilization, mechanical requirements, permitted processes, heat treatment and tests can differ. Never print an untested alternative standard on an MTC, and never treat a flat-sheet standard as finished-tube certification.

Chinese national steel material standards

NormTitle and product scopeRelevance to Dumai
GB/T 700Carbon structural steelsQ195/Q215/Q235/Q275 family; structure feedstock
GB/T 699-2015Quality carbon structural steels08, 10, 15, 20, 35, 45; chemistry-based engineering grades
GB/T 1591High-strength low-alloy structural steelsQ355 and related grades; edition and thickness dependent
GB/T 5213-2019Cold-rolled low-carbon sheet and stripDC01, DC03, DC04, DC05, DC06 forming family
GB/T 13237-2026Cold-rolled quality carbon steel sheet and stripCheck effective date and applicability for coil orders
GB/T 36399-2018Continuously hot-dip Al–Si coated steel sheet/stripCritical standard for DX grades with AS coating
GB/T 2518-2019Continuously hot-dip zinc and zinc-alloy coated sheetNOT the same as AS aluminium–silicon coating
GB/T 20878-2024Stainless steel designations and chemistryCurrent national stainless grade naming/chemistry
GB/T 3280-2015Cold-rolled stainless flat products300/400 stainless cold-rolled tube feedstock
GB/T 4237Hot-rolled stainless flat productsHot-rolled substrate, grade and delivery conditions
GB/T 222Chemical analysis permissible variationsProduct analysis tolerance framework
GB/T 228.1Metallic tensile test at room temperatureTensile/yield/elongation testing

Chinese carbon steel and cold forming grades

GradeNational normMechanical or grade meaningTube forming relevance
Q195GB/T 700Nominal yield classification around 195 MPaGeneral forming / welded mechanical tube feedstock
Q215GB/T 700Nominal yield classification around 215 MPaStructural applications by quality class
Q235A/B/C/DGB/T 700Nominal yield minimum ~235 MPa for thinner sectionsQuality and impact-testing variants
Q275GB/T 700Nominal yield classification around 275 MPaHigher strength, formability qualification
08/08AlGB/T 699 / GB/T 5213 product-dependentVery low-carbon gradesSoft forming and ERW
10/15/20GB/T 699Quality carbon steel, approx 0.10/0.15/0.20 C nameCheck heat analysis, deoxidation and condition
35/45GB/T 699Medium carbonHigher strength with more difficult welding
Q355GB/T 1591HSLA structural steelDo not substitute for Q235 without process/design review
DC01/DC03GB/T 5213-2019Cold-rolled commercial/drawingCorrespondence to EN same names only after edition tests
DC04/DC05/DC06GB/T 5213-2019Deep/extra-deep drawingLow yield, aging, r- and n-value matter

Cold rolled DC grades in Chinese GB/T 5213

GB/T 5213-2019 includes DC grades familiar from EN purchasing. For Chinese certification state GB/T 5213-2019 rather than merely DC01 or an assumed EN equivalence. Confirm product thickness, orientation, chemical maxima, yield and tensile values, elongation, r/n forming measures, surface quality and aging conditions on the actual mill certificate. Different national editions can specify different test conditions.

Chinese aluminum–silicon coated steel

Grade or coatingTechnical meaningPurchase verification
DX51D+ASCommercial formable substrateCoil grade under GB/T 36399-2018
DX52D+ASDrawing substrateConfirm availability and GB grade designation
DX53D+ASDeep drawing substrateStandard designation example explicitly uses DX53D+AS
DX54D+ASSevere forming qualityRelevant to Dumai DX54D+AS120 supply
DX55D+ASHigh formabilityCheck listed edition and mechanical performance
DX56D+ASEnhanced drawingHigher formability; welding must be qualified
AS8080 g/m² total nominal coating classConfirm test method and min spot values
AS120120 g/m² total nominal coating classCoating mass ≠ precise coating thickness
AS150150 g/m² total nominal coating classCheck availability, bend cracking and weld seam

The correct coating standard

GB/T 36399-2018 is the direct Chinese continuously hot-dip aluminium–silicon coated sheet and strip norm, applicable to the DX forming substrates with +AS. GB/T 2518-2019 covers Zn and Zn-alloy coatings and cannot be substituted for +AS. The Chinese standards committee also has a 2026 revision project combining metallic-coating standards, but a project is not itself an effective replacement of GB/T 36399-2018.

Coating verification

Request the exact Chinese standard/edition, steel substrate grade, coating code, minimum total coating mass, spot test convention, bend adhesion results, surface treatment, coil width/thickness, and process tolerances. Record whether the measured tube wall comprises base metal only; coating mass quoted for coil cannot certify finished-tube OD, weld seam corrosion or bend resistance.

Chinese stainless grades and cross-reference register

Chinese steel nameInternational screening nameFamilyKey chemistry
06Cr19Ni10304 / UNS S30400austeniticCr ~18–20; Ni ~8–11; C ≤0.08 (screening)
022Cr19Ni10304L / UNS S30403austenitic low carbonCr ~18–20; Ni ~8–12; C ≤0.03 (screening)
06Cr17Ni12Mo2316 / UNS S31600austenitic molybdenumCr ~16–18; Ni ~10–14; Mo ~2–3
022Cr17Ni12Mo2316L / UNS S31603austenitic low-C molybdenumMo ~2–3; C ≤0.03
06Cr18Ni11Ti321 / UNS S32100austenitic Ti stabilizedCr ~17–19; Ni ~9–12; Ti stabilization
06Cr18Ni11Nb347 / UNS S34700austenitic Nb stabilizedNb stabilization; heat analysis essential
015Cr21Ni26Mo5Cu2904L / UNS N08904 broad analoguehigh alloy austeniticCr/Ni/Mo/Cu high alloy; verify exact CN chemistry
022Cr11Ti409L familyferritic stabilized exhaustCr ~10.5–12.5; Ti; C low
06Cr13Al405 familyAl-alloyed ferritic stainlessCr ~11.5–14.5; Al alloying; NOT aluminized coating
06Cr17430 familyferritic chromiumCr ~16–18
022Cr18Ti439 familyTi-stabilized ferriticCr ~17–19; controlled Ti
019Cr19Mo2NbTi444 family / comparison onlyMo–Nb–Ti ferriticCr ~18–20; Mo ~2; Ti+Nb
019Cr19NbTi441-type comparison; confirm grade listingNb–Ti ferriticSpecific chemistry/order certification

China GB/T 20878-2024 governs national stainless steel designation and chemistry. Similar AISI/EN names in the table provide cross-search only; no cross-certification should be declared without simultaneously meeting the entire applicable foreign standard. Chinese stainless flat-product mechanical and surface requirements come from GB/T 3280-2015 or the appropriate hot-rolled flat norm.

300 series stainless grade register

AISI / tradeUNSEN screening cross-referenceMain tube relevanceIndicative chemistry, not acceptance limits
301S301001.4310 X10CrNi18-8austenitic; high work hardening; formed partsCr 16–18; Ni 6–8; C ≤0.15
302S302001.4319 (comparison only)austenitic; higher C than 304Cr 17–19; Ni 8–10; C ≤0.15
303S303001.4305 X8CrNiS18-9free-machining; sulfur; poor welding choiceCr 17–19; Ni 8–10; S ≥0.15
304S304001.4301 X5CrNi18-10general welded tube and fabricationCr 18–20; Ni 8–10.5; C ≤0.08
304LS304031.4307 / 1.4306lower carbon; welded assembliesCr 18–20; Ni 8–12; C ≤0.03
304HS304091.4948 (check product)elevated temperature; controlled carbonC 0.04–0.10; Cr 18–20; Ni 8–11
305S305001.4303 X4CrNi18-12deep forming; higher nickelCr 17–19; Ni 11–13
309SS309081.4833 X12CrNi23-13heat oxidation serviceCr 22–24; Ni 12–15; C ≤0.08
310SS310081.4845 X8CrNi25-21heat-resistant high chromium nickelCr 24–26; Ni 19–22; C ≤0.08
316S316001.4401 X5CrNiMo17-12-2molybdenum for chloride resistanceCr 16–18; Ni 10–14; Mo 2–3
316LS316031.4404 / 1.4432 / 1.4435welded chemical and hygienic tubesC ≤0.03; Cr 16–18; Mo 2–3
316TiS316351.4571 X6CrNiMoTi17-12-2Ti stabilized; hot serviceCr 16.5–18.5; Ni 10.5–13.5; Mo 2–2.5
317LS317031.4438 (comparison only)higher Mo; aggressive serviceCr 18–20; Ni 11–15; Mo 3–4
321S321001.4541 X6CrNiTi18-10Ti stabilized exhaust and heatCr 17–19; Ni 9–12; Ti controlled
347S347001.4550 X6CrNiNb18-10Nb stabilized weld/thermal applicationsCr 17–19; Ni 9–13; Nb controlled
904LN089041.4539 X1NiCrMoCu25-20-5high alloy austenitic; acid serviceCr 19–23; Ni 23–28; Mo 4–5; Cu 1–2

The chemistry column gives orientation ranges rounded from widely used specifications; acceptance requires the precise grade and edition’s chemical tables, product analysis tolerances and any agreed dual certification. EN variants under one US commercial name may have nonidentical nickel or molybdenum bounds.

400 series stainless grade register

AISI / tradeUNSEN screening cross-referenceMain tube relevanceIndicative chemistry, not acceptance limits
405S405001.4002 X6CrAl13Al-alloyed ferritic stainless; distinct from coated steelCr 11.5–14.5; Al 0.10–0.30
409S409001.4512 X2CrTi12Ti stabilized; exhaust componentsCr 10.5–11.75; C ≤0.08; Ti stabilization
409LS40910 / EN variant1.4512 comparisonlow-C exhaust; check grade-specific producer chemistryExact chemistry depends designation
410S410001.4006 X12Cr13martensitic; may be heat treatedCr 11.5–13.5; C ≤0.15
410SS410081.4000 X6Cr13low-C ferritic counterpartCr 11.5–13.5; C ≤0.08
420S420001.4021 / 1.4028 variantsmartensitic; wear/hardness applicationsCr 12–14; C varies materially
430S430001.4016 X6Cr1717% chromium; household/ductingCr 16–18; Ni not specified as alloy addition
430Tivaries1.4510/1.4520 comparison onlystabilized ferritic; specify exact designationCr ~16–18; Ti controlled
434S434001.4113 X6CrMo17-1Mo-bearing ferritic corrosion upgradeCr 16–18; Mo ~0.75–1.25
436S436001.4526 comparisonMo-bearing and stabilized exhaust optionCr 16–18; Mo ~0.75–1.25
439S430351.4510 X3CrTi17Ti stabilized; exhaust and exchangersCr 17–19; Ti controlled
441S43940 / S439321.4509 X2CrTiNb18dual stabilized Ti+Nb; elevated-temp exhaustCr ~17.5–18.5; Ti+Nb controlled
444S444001.4521 X2CrMoTi18-2Mo-bearing ferritic; high corrosion resistanceCr 17–20; Mo 1.75–2.5
446S446001.4749 comparisonhigh-Cr oxidation resistanceCr 23–27

The 400 series spans ferritic and martensitic alloys. 409, 430, 439, 441 and 444 are ferritic; 410 and many 420 variants are martensitic. They cannot be substituted by series number alone. Stabilization is essential to welding and heat-resistance performance.

Special study 409AL and aluminized stainless

Two different uses of a similar name

In exhaust purchasing, “409AL”, “409 Aluminized” or “aluminized 409” commonly describes a 409 ferritic stainless substrate with hot-dip Al–Si coating (often Type 1), supplied as coated strip under ASTM A463/A463M or an agreed equivalent manufacturing specification. In other metallurgical contexts “409Al” may designate an aluminum-stabilized ferritic alloy rather than a surface-coated product. The suffix AL is not a safe stand-alone specification or universally standardized UNS grade.

CheckRequired PO or MTC statement
SubstrateUNS S40900 / other explicitly specified 409 family grade; separate heat analysis
CoatingAl–Si Type 1 vs pure-Al Type 2; applicable sheet standard or mill technical specification
Coating massExact T1 / T1M or EN AS designation, total-both-sides vs per-side convention
Finished tubeTube standard, process (ERW, TIG/laser), OD, wall and length tolerances
WeldTreatment of weld seam and local coating loss; corrosion qualification if required
VerificationCoating mass/thickness; adhesion; substrate PMI; tube dimensional and leak tests

A 409 substrate with aluminized coating is neither plain aluminized carbon steel nor bare 409 stainless. The coating may be damaged or absent at the weld seam and cut ends; agree on treatment and service testing. The producer should specify coating condition after tube forming, not only before it.

Chinese mill certificate checklist by material

Product groupMinimum mill document fieldAdditional decisive check
Carbon Q235/Q355Heat, chemical analysis, tensile, impact category if orderedExact structural steel quality and thickness interval
Cold rolled DC01–DC06Re/Rp, Rm, A80, r and n where applicableSurface finish, formability, strain aging
DX54D+AS120Substrate grade and coating designation and massAl–Si coating adherence and after-forming condition
300 series SSGB/T 20878 chemistry + flat-product standard + surfaceWeld sensitization, PMI, solution anneal when relevant
400 series SSCr/C/N/Ti/Nb/Mo chemistry, annealed temperWeld HAZ, embrittlement and surface oxidation
409ALIdentify whether coated 409 stainless or Al-stabilized gradeSeparate substrate chemistry and coating evidence

Tube purchase-order specification matrix

FieldWhat an engineering inquiry or PO must state
ProductWelded round tube; intended mechanical, exhaust, heat-exchanger or pressure duty
Base gradeExact material designation and source sheet/strip standard + edition
CoatingNone / Al–Si / Al / Zn–Al; mass, type, both-face convention, coil condition
Tube standardApplicable finished-product norm and edition; do not infer from strip grade
DimensionsOD x nominal wall x cut length; tolerances, eccentricity, straightness, ovality
ProductionHF-ERW / laser / TIG; weld-bead treatment; anneal/pickling/passivation if relevant
VerificationChemistry, tensile or hardness, flattening/flaring/bend, leak/eddy/UT where applicable
CertificationEN 10204 3.1 or other agreed inspection certificate; heat/coil/tube traceability
PackingBlue-wrapped bundles, without pallet/sleeve/slings if requested; moisture protection

Tube manufacturing and acceptance checks

Coil receipt

Record heat number, coil number, coating face/mass, thickness, tensile condition and supplier MTC. A tube made from a compliant coil is not automatically a compliant tube.

Slitting and forming

Confirm strip edge condition, strip width, springback, seam orientation, and coating crack tolerance. High-strength sheet may have limited formability.

Weld process

Identify HF-ERW, TIG or laser; assess weld speed and heat input, seam bead and heat-affected region. High-Cr ferritic tubes need controlled welding and may require post-weld treatment.

Dimensional checks

Measure OD, nominal and minimum wall, out-of-roundness, length, straightness, end squareness and bend/ovality where specified. Use the actual tube standard tolerances.

Nondestructive/leak testing

Apply the specific test prescribed or agreed for the product: eddy-current, ultrasonic, pneumatic or hydrostatic. An inspection technology is not a substitute for the required acceptance level.

Marking and documentation

Record manufacturer, standard, grade, size, batch/heat and inspection results. Any claim to ASTM, EN or GOST should be supported by all relevant mandatory tests.

Primary sources

https://openstd.samr.gov.cn/bzgk/std/newGbInfo?hcno=192F05BCCC66349370A28EDF0CC742EA

https://openstd.samr.gov.cn/bzgk/std/newGbInfo?hcno=9ABAE7D4AB43B1B3F78BAF65B9C6291F

https://openstd.samr.gov.cn/bzgk/std/newGbInfo?hcno=8B23C177DDD1CF1F010206D48DAAC71D

https://openstd.samr.gov.cn/bzgk/std/newGbInfo?hcno=D70887EA9D2E0DEDA308A4177EE4B81C

https://openstd.samr.gov.cn/bzgk/std/newGbInfo?hcno=9F80F33DB9597FB0C628094B1525042F

Back to Insights

Scan the code to connect.